Why Fabric Fails Lightfastness Testing
Learn why nylon fabric failed AATCC TM16.3 testing, how lightfastness differs from UPF, and why the approved specimen must represent bulk production.
FABRIC TESTING


A fabric can fail lightfastness testing after development approval for two different reasons: the final material does not retain its color under the required exposure, or the approved specimen does not represent bulk production.
Both problems occurred in a dark army green, 100% nylon project. The customer required Grade 4 or above under AATCC TM16.3. The fabric initially fell below Grade 4, then achieved Grade 4 or above after the bulk material was refinished and retested by the same method.
A test-only length had also been exposed to sunlight before submission. That specimen passed, while the untreated bulk fabric failed. Its result could not be used to approve the bulk.
What a Lightfastness Failure Actually Means
Lightfastness describes a textile color’s resistance to change under specified light exposure.
AATCC TM16.3 evaluates colorfastness to light using xenon-arc exposure. Its options apply to textile materials and to the colorants, finishes, and treatments applied to them.
A fabric fails when the color change exceeds the buyer’s acceptance limit. Grade 4 or above was the requirement for this project; it is not a universal requirement for nylon or outdoor apparel.
Specify the test option, exposure conditions, evaluation criteria, and minimum grade as well as the method number. A xenon-arc result cannot be converted directly into a guaranteed number of days or months outdoors.
Why Fabric Fades in Sunlight or Xenon-Arc Testing
Several factors can affect fading in sunlight or a xenon-arc test:
Fiber composition
Dye and colorant selection
Color recipe
Shade depth
Dyeing process control
Heat history
Subsequent finishing
The specified exposure and evaluation conditions
“Army green” identifies a color family, not a performance specification. Two dark army green fabrics can use different dye combinations, processing conditions, and finishes.
In CC Textile’s experience, dark army green needs careful shade assessment. In a mixed shade, colorants that respond differently to light can produce a noticeable change in hue.
This does not mean all army green nylon will fail. Test the actual color and final finish rather than relying on a shade name or an earlier lab dip.
UPF Is Not the Same as Colorfastness to Light
UPF and lightfastness measure different properties.
AATCC TM183 measures the ultraviolet radiation transmitted through or blocked by fabric intended for UV protection. AATCC TM16.3 assesses color change after xenon-arc exposure.
A fabric can meet a UV-protection requirement and still fail lightfastness testing. It can also have acceptable lightfastness without a specified UPF rating.
For the dark army green nylon, the team used the selected UPF finish and checked lightfastness separately. The before-and-after AATCC TM16.3 reports showed:
Before finishing: below Grade 4
After finishing: Grade 4 or above
The improvement applies to that fabric, dye recipe, and processing route. It does not establish that every UPF finish improves lightfastness. Specify and test the two properties separately for each new color or construction.
When the Approved Test Sample Does Not Represent Bulk
The submitted specimen must represent the material being approved. In this project, a two-meter test length had been exposed to sunlight before submission, changing the dark army green to a noticeably paler, whitish green.
That length passed, but bulk fabric without the same pre-exposure failed. The test specimen no longer represented the bulk color and finishing condition.
Undisclosed preconditioning can create several problems:
The report cannot be reliably connected to the production lot.
The approved sample may differ visibly from the required bulk shade.
Bulk inspection or garment testing can reveal the failure later.
Re-finishing and repeat testing can delay delivery.
The buyer may have a passing report without having compliant bulk fabric.
Record any conditioning required by the agreed method. A treatment applied only to the test length cannot verify the performance of bulk fabric that did not receive it.
The same principle applies to other tests. Our guide to outdoor fabric testing and garment failure explains why a result applies to the submitted specimen and test conditions, rather than automatically to every roll or garment.
How the Bulk Fabric Was Corrected
The dark army green, 100% nylon bulk fabric required corrective processing because it had not met the agreed AATCC TM16.3 Grade 4 minimum.
The actual bulk fabric was refinished with the selected UPF finish, then retested under the same AATCC TM16.3 method. The result reached Grade 4 or above.
The corrective action covered:
Re-finishing the actual bulk fabric
Testing the final finished material
Using the same lightfastness test method
Confirming a result of Grade 4 or above
Retesting the finished bulk confirmed the correction. An earlier development report could not have done so, and a different nylon construction, color recipe, or finish would still need its own evaluation.
What Buyers Should Specify Before Testing
“Good lightfastness” leaves the acceptance criteria undefined. Before bulk ordering, agree on measurable requirements:
Fabric composition and construction
Approved color reference or lab dip
Lightfastness test method and applicable version
Test option and exposure conditions where required
Minimum acceptable color-change grade
Required finishing route
The production stage at which testing will occur
Whether the specimen must be taken from final finished bulk
How the production lot, roll and cutting location will be recorded
Whether any pre-conditioning is permitted
Retesting and corrective-action requirements
Whether written approval is required before shipment
If UV protection is also required, specify its method, target, and conditions separately. A lightfastness result does not establish a UPF rating.
Our quality and compliance process connects the approved specification, final finishing route and required testing with bulk production.
Include Finishing and Testing in the Quote
A lower quote is not necessarily a sign of poor quality. Compare quotes that include the same finish, testing, and production controls.
Finishing chemicals, processing, and quality control all add cost. If the required treatment was excluded from the quote, the supplier may need to renegotiate the price, absorb the cost, or risk leaving part of the approved process incomplete.
For the buyer, an omitted requirement can lead to:
Bulk lightfastness failure
Re-finishing costs
Additional laboratory testing
Color changes after corrective processing
Garment production delays
Missed shipment dates
Disputes over responsibility
Refinishing bulk fabric or delaying garment production can cost far more than the initial fabric saving.
Confirm that the quote covers the agreed finish, bulk testing, and responsibility for corrective action.
A Practical Lightfastness RFQ Requirement
An RFQ for this project could state:
100% nylon woven fabric in dark army green. Lightfastness to be tested according to AATCC TM16.3 using the mutually agreed option and exposure conditions. Required color-change result: Grade 4 or above. The submitted specimen must be selected from final finished bulk production, and any pre-conditioning must be declared. UPF performance, if required, must be specified and tested separately.
Check the final wording against the garment application, customer manual, and appointed laboratory’s requirements.
Keep the Test Report and Bulk Fabric Traceable
The report, specimen, and bulk lot must refer to the same construction, color, and finishing condition.
The dark army green nylon project showed three separate lessons:
UPF and lightfastness are different properties.
A project-specific finish may affect both, but the result must be verified.
A passing test-only specimen does not approve bulk fabric when the specimen is not representative.
Use a fabric sample, color standard, AATCC requirement, or previous failure report to discuss the fabric development plan before bulk production.
Contact CC Textile to review the project. Follow CC Textile on LinkedIn for fabric-development and testing notes.
Frequently asked questions
What does AATCC TM16.3 test?
It evaluates textile colorfastness under specified xenon-arc exposure. Also define the test option, exposure conditions, and minimum acceptable color-change grade.
Is UPF finishing the same as improving fabric lightfastness?
No. UPF concerns UV transmission, while lightfastness concerns color change under light exposure. A particular finish may affect both, but each property needs separate verification.
Why can a fabric test sample pass while the bulk fabric fails?
The specimen may represent a different lot, processing stage, or finish. Undisclosed preconditioning can also make it unrepresentative. Approve bulk using a traceable specimen from the final finished production.
Why does dark army green nylon fail lightfastness testing?
There is no single cause. Fiber, dye selection, shade recipe and depth, dyeing control, and finishing can all affect the result. Test the actual color and final finished fabric against the agreed requirement.